Paper properties
Property |
Value (SI)
|
Value (US) |
Test method |
Grammage
|
52 ± 3 |
g/m² |
13.8 ± 0.8 |
17x22 - 500 lbs |
ISO 536 |
Thickness
|
53 ± 5 |
µm |
2.09 ± 0.20 |
mils |
ISO 534 |
Moisture, PM
|
6.0 ± 1.0 |
% |
|
|
ISO 287 |
ISO Brightness C/2°, CS
|
82 ≥ 78 |
% |
|
|
ISO 2470 |
Opacity
|
74 ≥ 70 |
% |
|
|
ISO 2471 |
Roughness PPS 10, CS
|
1.3 ≤ 2.2 |
µm |
|
|
ISO 8791-4 |
Roughness PPS 10, RS
|
5.2 ≤ 6.1 |
µm |
|
|
ISO 8791-4 |
Tensile strength (MD)
|
3.9 ≥ 2.8 |
kN/m |
22.3 ≥ 16.0 |
lbf/in |
ISO 1924-3 |
Tensile strength (CD)
|
1.7 ≥ 1.3 |
kN/m |
9.7 ≥ 7.4 |
lbf/in |
ISO 1924-3 |
Tear strength (MD)
|
320 ≥ 200 |
mN |
32.6 ≥ 20.4 |
gf |
ISO 1974 |
Tear strength (CD)
|
370 ≥ 250 |
mN |
37.7 ≥ 25.5 |
gf |
ISO 1974 |
Unger oil absorption, CS
|
0.8 ≤ 1.0 |
g/m² |
|
|
SCAN-P37 (60 sec) |